Super - Duplex S32750 Tilsiz trubka 8 × SCH40s
Aug 26, 2025
Xabar QOLDIRISH
Ikki dumble zanglamaydigan po'lat - bu ferrit va achinitdan iborat Super Dupleks po'lat. Gne turli xil shakllarni ta'minlaydi: plitalar, naychalar, novdalar, ro'mollar, profillar va hokazolar va payvandlangan naychalar mavjud. Gneda boy mahsulotlar bor, sozlashni qo'llab-quvvatlaydi, o'z fabrikasi, bitta -}}}}}}}}}}}} SAKTHEVE xizmat, bepul QUNGOG! Va Xitoyda GNEE kompaniyasining tashrifiga tashrif buyuring! Elektron pochta:sales@gneestainless.com
Quyida bizning laboratoriyalarimiz har bir issiqlik bilan ta'minlanadi, standartdan tashqari rioya qilinishini ta'minlaydi.
1. Kimyoviy (WT%, dastada tahlili)
CR 25.0-26.5|Ni 6.0-7.0|MO 3.5-4.5|N 0.24-32|Prien 42.0 dan katta yoki unga teng
2. Mexanik konvert (RT, bo'ylama)
RP0.2 550 MPa dan katta yoki teng RM 800 - 1 000 MPA|25% dan katta yoki teng|Kv (-46 daraja) 45 j dan katta yoki teng
3. Korroziya qarshiligi
ASTM G48 usuli 24 h @ 50 darajadan keyin <1 gm⁻²
ASTM G48 usuli C tanqidiy tanqidiy harorat 80 darajadan katta yoki unga teng
4. Mikroektura nazorati
Asm e562 Ferrit 45-55%, ASTM E112 Don hajmi 6-8, zararli s dvimental s, χ, fazalari (versiyalari orqali tasdiqlangan)
5. O'lcham va NDT protokoli
• OD tolizatsiyasi ± 0,5%, devor ± 10%
• 100% (ASTM E213) + 100% ET (ASTM E571)
• gidrostatik 1,5 × dizayn bosimi, 10 s taglik
6. Hujjatlar to'plami
• DNV markali en 10204 3.2
• Issiqlik jadvali, PMI xaritasi, Charpy Curlari, G48 korroziya to'g'risidagi hisobot
Joriy Ex - Stokom: 40 t Candom 12 m uzunligi, tekis uchlari, darhol tuzlash / passivatsiya yoki so'rov bo'yicha 3LPP bilan qoplangan.
Mtr to'plami yoki uchinchi - partiyasi nazorati uyasi:
2507 moddiy ro'yxatni olish uchun bosing