Zanglamaydigan po'latdan 304L darajasi - past karbonli korroziyaga chidamli

Feb 05, 2026

Xabar QOLDIRISH

Stainless Steel Grade 304 - Food Grade & Corrosion ResistantStainless Steel Grade 2205 - Duplex High Strength GradeStainless Steel Grade 430 - Magnetic Stainless Steel Grade

Zanglamaydigan po'latdan kimyoviy tarkibi 304

1-jadval.304 zanglamaydigan po'latdan yasalgan qotishmalar uchun kimyoviy tarkibi

%

304

304L

304H

C

0.0 - 0.07

0.0 - 0.03

0.04 - 0.08

Mn

0.0 - 2.0

0.0 - 2.00

0.0 - 2.0

Si

0.0 - 1.00

0.0 - 1.00

0.0 - 1.0

P

0.0 - 0.05

0.0 - 0.05

0.0 - 0.04

S

0.0 - 0.03

0.0 - 0.02

0.0 - 0.02

Cr

17.50 - 19.50

17.50 - 19.50

17.00 - 19.00

Ni

8.00 - 10.50

8.00 - 10.50

8.00 - 11.00

Fe

Balans

Balans

Balans

N

0.0-0.11

0.0-0.11

0.0 - 0.10

 

304 zanglamaydigan po'latning xususiyatlari

Zanglamaydigan po'latning mexanik xususiyatlari 304

Jadval 2a.Qalinligi 8 mm gacha bo'lgan 304 zanglamaydigan po'latdan yasalgan - varaq uchun mexanik xususiyatlar

Baho

304

304L

304H

Kuchlanish kuchi (MPa)

540 - 750

520 - 700

-

Ishonchli stress (MPa)

230 min

220 min

-

Cho'zilish A50 mm

45 min %

45 min %

-


Jadval 2b.Qalinligi 8 - 75 mm dan 304 zanglamaydigan po'latdan yasalgan - plastinka uchun mexanik xususiyatlar

Baho

304

304L

304H

Kuchlanish kuchi (MPa)

520 - 720

500 - 700

-

Ishonchli stress (MPa)

210 min

200 min

-

Uzayish A5

45 min %

45 min %

-


Jadval 2c.304 zanglamaydigan po'latdan yasalgan qotishmalar uchun mexanik xususiyatlar - bar va diametri 160 mm gacha / qalinligi

Baho

304

304L

304H

Kuchlanish kuchi (MPa)

500 - 700

500 - 700

500 - 700

Ishonchli stress (MPa)

190

175 min

185 min

Cho'zilish A50 mm

45 min %

45 min %

40 min %

Brinellning qattiqligi

215 maksimal HB

215 maksimal HB

-

So'rov yuborish